Construction and steps of a mixer for testing the demulsification speed of emulsified asphalt
Date: 2024-08-22Read: 11

1、 Emulsified asphalt emulsion breaking speed test mixer product structure:

The emulsified asphalt emulsion breaking speed test mixer consists of an electric motor and a stirring blade. The motor drives the stirring blade to rotate, allowing the material to achieve mixing and mass transfer (dissolution, extraction, absorption).Developed and researched the "Mixing Test of Emulsified Asphalt and Mineral Aggregate", which also meets national standards and relevant standards in the petrochemical industry

TD659-2The electric emulsified asphalt and mineral aggregate mixing tester is suitable for mineral aggregate and lotion with specified gradation25℃±1℃Mixing under conditions,

2、 Experimental steps

1、Sift and grade the aggregate (stone chips) used in the actual project, and weigh and mix them according to the proportion in Table T0658-1 into two standard graded mineral materials, each weighing 200g

Proportion of mineral particle test for mixing test (%)

Mineral material specifications(mm)

Agroup

Bgroup

<0.075

3

10

0.3~0.075


30

0.6~0.3

5

30

2.36~0.6

7

30

4.75~2.36

85

——

total

100

100

2Sift and grade the aggregate (stone chips) actually used in the project, and weigh and mix them into two standard graded mineral materials each weighing 200g according to the proportion in Table T0658-1.

3Wash the mixing pot thoroughly and dry it.

4. Mix 200g of group A mineral aggregate evenly in the mixing pot. When it is cationic emulsified asphalt, first inject 5ml of distilled water to mix well, and then inject 20g of lotion. When it is anionic emulsified asphalt, directly inject 20g of lotion, mix it with a metal spoon at a speed of 60r/min for 30s, and observe the uniformity of mineral aggregate and lotion after mixing.

5Mix the ingredients in the mixing potBGroup mineral materials200gAfter mixing evenly, inject30mlDistilled water, mix well, and pour in50gLotion sample, then continue to use a metal spoon to60r/minThe speed of mixing60sObserve the uniformity of mineral aggregate and lotion after mixing.

6Determine the demulsification speed of samples according to the mixing uniformity of two groups of mineral aggregate and lotion samples as shown in the following table.


AMixing results of group mineral materials

BMixing results of group mineral materials

Demulsification speed

code name

The mixture is in a loose state, and some mineral particles are not coated with asphalt. The distribution of asphalt is not uniform, and some aggregate into clumps

Immediately after asphalt in lotion is mixed Clumped together, unable to mix

Quick crack

RS

Mix the mixture evenly

The mixture is in a loose state, and the distribution of asphalt is not uniform enough, with some clumping together

Mid split

MS


The mixture is pasty, and the asphalt lotion is evenly distributed,

Slow cracking

SS